Specification versus Shop Floor: Where the Gap Opens

The drawing says a nominal wall of 2.5 mm with a tolerance of ±0.1 mm. The resin datasheet lists a mold shrinkage of about 1.6%. The quotation assumes a single cavity, one gate, and a 35-second cycle. None of those three documents says anything about the top surface directly above the internal boss, which is exactly where the first sample shows a soft depression roughly 0.12 mm deep after twenty minutes on the bench.

How to Diagnose and Prevent Sink Marks in Injection Molding
How to Diagnose and Prevent Sink Marks in Injection Molding

That gap between the paperwork and the part is where sink marks live. The step that decides most of these cases is one line in the process sheet: hold time. It is also the line most often copied from the previous job and never verified. A molding team that checks gate seal before arguing about cavity pressure, material, or tool geometry usually resolves the problem in an afternoon; a team that starts by adding pressure often creates flash, warpage, and a part that fails somewhere else instead.

The workflow that actually works runs in a fixed order: confirm the design's thickness map, verify when the gate seals, balance cooling at the thick zone, then correct the tool only if the first three steps leave no room. Everything below follows that sequence.

What a Sink Mark Actually Is

A sink mark is a localized surface depression caused by volumetric shrinkage that packing pressure can no longer compensate. The outer skin freezes first. The core beneath it keeps shrinking as it cools. If the gate has already sealed, no fresh melt can replace that lost volume, and the still-soft surface is drawn inward.

Three conditions normally combine: a section that is thicker than the surrounding wall, a gate that seals before packing is complete, and cooling that keeps the thick zone molten after the rest of the part has stiffened. Remove any one of them and the depression either disappears or drops below the cosmetic limit.

Two related defects are frequently confused with it. A void is an internal cavity with the same shrinkage origin, but the surrounding skin is stiff enough that the surface does not deflect, so the shrinkage appears as a bubble inside the section. Splay or silver streaking from moisture is a surface appearance problem with an entirely different cause. Treating either as a packing deficiency leads to over-packing, which buys flash and residual stress without fixing anything.

The Parameter Most Often Skipped: Hold Time to Gate Seal

Hold time is the least verified setting on most presses. It is usually set to "long enough" — three seconds, five seconds, whatever the last job used — with no check of whether the gate is open at that moment. If the gate freezes at 2.2 seconds and the timer runs for 5, more than half of the hold phase is loading the sprue and nothing else. If the gate seals at 6 seconds and the timer runs for 3, the final portion of packing never happens, and the sink shows up at the far end of flow or over the thickest section.

The correction is a gate seal study, and it costs less time than the meeting it prevents.

Injection Molding Sink Marks: A HYNEU Manufacturing Guide
Injection Molding Sink Marks: A HYNEU Manufacturing Guide

Running a Gate Seal Study

  • Establish a stable baseline process and record melt temperature, mold temperature, injection profile, and transfer position.
  • Run a ladder of hold times — 1, 2, 3, 4, 5, 6, and 8 seconds — changing nothing else.
  • At each step, allow 10 to 15 shots for stabilization, then weigh five consecutive parts on a balance readable to 0.01 g for small components.
  • Plot average part weight against hold time. Weight climbs steeply, then flattens. The knee of that curve is the point where the gate seals.
  • Set production hold time slightly beyond the knee, typically 0.5 to 1.0 second past it, so normal shot-to-shot variation does not drop parts below the plateau.
  • Repeat the study after a material, color, or melt temperature change. A different viscosity moves the seal point, and a setting that was correct last month may not be correct now.

On an instrumented tool, cavity pressure at the gate end drops to zero at the same moment, and the curve can be read directly. Most tools in general production are not instrumented, and the weight method gives the same answer with a balance and an hour of press time.

One outcome deserves attention: if the weight curve never flattens within the hold time the machine or cycle can realistically provide, the gate is too small for the section being packed. That is a tooling problem, and no parameter change will solve it.

Geometry Sets the Ceiling on Process Corrections

Process can compensate for geometry only inside a window. Once that window is exhausted, more pressure does not close a sink; it moves the failure somewhere else.

Ribs, Bosses, and Corners

Most design guidance places rib thickness at 0.5 to 0.6 times the adjoining wall. Above that ratio, the rib behaves as a thick section: it holds heat longer, shrinks later, and pulls the opposite face with it. The sink then appears directly over the rib root, on the cosmetic side, which is the worst possible location. Coring the rib, thinning it, or adding a small radius at the root while reducing thickness are the standard responses.

Bosses follow the same logic. A boss wall as thick as the nominal wall, or a solid boss, retains far more heat than the surrounding material. Reducing boss wall thickness, coring deeper, or replacing a large boss with a smaller one plus gussets addresses the cause. There is a detail that catches even experienced designers: a generous fillet at the base of a rib or boss adds mass precisely where shrinkage is worst. The radius helps stress concentration and hurts cosmetics unless the rib is thinned at the same time.

Gate Size and Location

A gate that is too small freezes early and cuts off packing for the entire cavity. On thick parts, gate size is often driven by packing rather than filling, so the flow-length calculation alone will undersize it. Gate position matters as much as size, because packing pressure decays with distance; a thick section at the end of the flow path sinks before an identical section near the gate.

Multi-gate layouts and valve gates give more control but create weld lines, and a weld line across a visible surface is a separate problem with a separate fix. Gate count and gate type are best decided while a sink risk map is still on the table, not after T1 samples come back with depressions.

Diagnosis by Location and Timing

Where the depression sits tells you more than any single parameter reading. A sink directly opposite a rib or boss points to geometry. A sink close to the gate points to early gate freeze or short packing. A sink at the far end of flow points to pressure loss through a thin gate or a cold mold. A depression that only becomes visible a day after molding points to post-molding shrinkage, which is a material and acceptance-timing issue rather than a press setting.

Observed conditionLikely mechanismHow to verifyFirst corrective step
Depression on flat face opposite a ribRib-to-wall ratio too high; local mass holds heatMeasure rib and wall thickness on the CAD and on a cut sampleThin the rib, core it out, adjust packing as an interim measure
Sink at a bossBoss wall thickness or solid sectionSection the boss, check core depth and wall thicknessReduce boss wall, core deeper, add gussets
Sink near the gateGate sealed before packing completedGate seal study using part weight versus hold timeExtend hold time, then review gate size
Sink at the far end of flowPressure loss through a small or cold gateCompare part weight across the ladder; check fill-end pressure if instrumentedEnlarge or relocate the gate, add a second gate
Surface depression with an internal cavity in a heavy sectionVoid rather than a classic sinkCut a part or use non-destructive scanning; compare part densityReduce section thickness, extend packing, reposition gate
Sink visible 24 to 48 hours after moldingPost-molding shrinkage in semi-crystalline resinRe-measure the same parts after stabilization at controlled temperatureConfirm drying, review grade, define acceptance timing

The Correction Ladder

Corrections should be applied in order of cost and reversibility. Jumping to the bottom of the list is how a cosmetic issue becomes a tool modification and a schedule slip.

  • Confirm gate seal time and extend hold time past the knee. This is free and fixes a large share of cases.
  • Check the cushion. If the screw bottoms out, cavity pressure varies from shot to shot and the sink appears intermittently, which is often misread as a material problem.
  • Balance cooling at the thick zone. A baffle or bubbler in a boss, or a separate cooling circuit for a heavy section, changes the local solidification time without touching the rest of the cycle.
  • Adjust melt and mold temperature within the material window. A modest mold temperature increase in the thick area slows skin formation and extends the packing window, at the cost of cycle time.
  • Raise hold pressure only after the steps above. Over-packing introduces flash, sticking, warpage, and high molded-in stress that shows up later as cracking or dimensional drift.
  • Resize or relocate the gate. This is a tool change with a cost, a lead time, and a requalification requirement.
  • Change material or geometry. A filled grade or a design revision is the last resort, and both need customer approval and a fresh first-article review.

Material and Drying Effects That Get Misdiagnosed

Semi-crystalline resins such as PP, PE, PA, and POM shrink more and sink more readily than amorphous resins such as ABS or PC, because the volume change on crystallization is larger. Glass-filled grades reduce shrinkage and sink tendency, but they bring directional shrinkage and stronger weld lines; trading a sink for a warp is not an improvement.

Moisture is a separate cause that occasionally gets blamed on packing. Undried PA, PC, and PBT show splay, silver streaks, and sometimes a rough patch that resembles a surface depression until it is examined under magnification. If dryer performance has not been verified, no amount of hold pressure will improve the surface.

Regrind ratio also shifts shrinkage, particularly in filled materials where fiber length degrades on each pass. A job that ran clean at 10% regrind can show sink at 25% with no change to the press settings at all. When a defect appears without a process change, the material lot and regrind ratio are the first records to pull.

Inspection, Acceptance Criteria, and Timing

Sink marks are rarely called out on a drawing, which is why they cause so many late disputes. The practical answer is a cosmetic standard agreed at T1 and signed by both sides, covering lighting, viewing distance and angle, and the measurement method. A common convention is inspection under roughly 500 lux with the viewer at about 45 degrees, but the exact condition matters less than the fact that both parties use the same one.

Surface finish is a factor buyers underestimate. A fine matte texture hides a depression that would be obvious on a polished, high-gloss surface. If the same tool is later run in a gloss variant, a sink that passed on texture may fail immediately.

Where a number is required, measure with a dial indicator on a surface plate or a straight edge and feeler gauge. Where a visual standard is enough, compare against a signed limit sample. Either way, record the time after molding in the inspection plan, because a part measured at ten minutes and the same part measured at 24 hours can give different results in semi-crystalline resins.

What Procurement Should Confirm Before Tooling Is Cut

For buyers sourcing injection molded components, sink marks are cheap to prevent and expensive to find at incoming inspection. The useful questions are mostly about documentation, and they are best asked before the purchase order, not after the first shipment.

  • A DFM report that maps nominal wall and flags ribs, bosses, and corners that exceed the recommended thickness ratio.
  • Gate seal data from T1 or T2 sampling, not just a parameter sheet copied from a similar project.
  • A cosmetic acceptance standard with signed limit samples, including the lighting condition and viewing angle.
  • Inspection timing after molding, stated explicitly for semi-crystalline materials.
  • Change control covering gate, cooling, and material changes that require re-qualification.
  • Clear agreement on who bears the cost of a tool modification when the change is driven by design rather than process.

The last item causes more delay than the technical work itself. Resizing a gate is a tool modification with a cost and a lead time. Agreed at T1, it is a line in the sample report; discovered in week two of mass production, it is a schedule problem and an invoice problem together. With resin pricing and tooling lead times still moving through 2026, pulling that decision forward is worth more than shaving a day off the sampling schedule.

From the manufacturing side, the conclusion is unglamorous. Sink marks are not solved by a single parameter or a better press. They are controlled by checking gate seal before debating pressure, by designing ribs and bosses that do not hoard heat, by cooling the thick zone deliberately, and by agreeing on what "acceptable" looks like while the tool is still open for modification. That sequence is what separates a T1 sample that needs one adjustment from a project that spends a month arguing about a surface no drawing ever specified.