On a molding card, holding pressure can look like one of the easiest settings to copy: a single value, a number of seconds. On the shop floor, it is rarely that simple. The same holding pressure that removes a sink mark can cause flash. The pressure that holds a critical dimension can leave residual stress inside the part, and the part can move after ejection. In plastic injection holding pressure, the real task is not to “add more pressure.” It is to manage the relationship between pressure, time, gate freeze, part weight, and dimensional response.

What Is Holding Pressure in Injection Molding?

At the end of the filling stage, the screw reaches a set transfer position and the machine switches from velocity control to pressure control. From that point on, the screw no longer pushes the melt forward at filling speed. It maintains a controlled pressure against the melt in front of the screw. That second-stage pressure is called holding pressure.

Packing Pressure Explained: Sink Marks, Warpage, and Dimensional Control
Packing Pressure Explained: Sink Marks, Warpage, and Dimensional Control

In many machine controllers, holding pressure is also called packing pressure or second-stage pressure. Some suppliers split it into a higher initial pack pressure and a lower follow-up holding pressure. The practical function is the same: to push a small amount of molten polymer into the cavity while the material cools and shrinks.

Holding pressure is not intended to fill the cavity. Filling should be nearly complete at switchover. If the part is under-filled before pressure control begins, the problem is usually the switchover position, shot size, or melt flow. Using holding pressure to fill an under-packed cavity leads to unstable weight, pressure variation, and poor cycle repeatability.

How Packing Pressure Affects Part Quality

Shrinkage and dimensional tolerance

As polymer cools, it contracts. Holding pressure compensates for part of that volumetric shrinkage by keeping the melt compressed against the cavity walls. Higher holding pressure normally increases part weight, reduces linear shrinkage, and helps hold dimension. But the relationship is not linear.

The area near the gate can become overpacked while the far end of the cavity remains under-packed. That is why a part may be within tolerance at one measuring point and outside it at another. Once the gate freezes, the cavity is sealed from the screw. Additional holding time after gate freeze no longer changes dimensions or weight.

Sink marks and surface defects

Holding Pressure in Injection Molding: What Your Drawing Never Tells You
Holding Pressure in Injection Molding: What Your Drawing Never Tells You

Sink marks appear when the surface of a thick section collapses because the inner material shrinks faster than the outer skin can support. Packing pressure helps feed melt into the thick section before the gate freezes. If a part still shows sink marks, check gate size and rib design before continuing to raise pressure. A thin or early-freezing gate cannot deliver pressure into the cavity no matter how high the machine setting is.

Flash and mold load

High holding pressure increases cavity pressure and works against the clamping force. If the mold is old, poorly vented, or has worn parting line seals, increased packing pressure can cause flash at the parting line, insert edges, and ejector pin clearances. Overpacking can also damage the mold slowly over many cycles. When changing holding pressure, inspect the parting line and compare the pressure setting with the selected machine clamp tonnage.

Residual stress and warpage

Packing pressure compresses and slightly orients polymer molecules, especially near the gate area. If the part is packed unevenly, different regions cool at different densities. After ejection, that difference can release as warpage or distortion. A single high holding pressure may solve sink marks but make flatness worse. For large flat panels, a pressure profile often performs better than a constant high pressure.

Starting Values for Holding Pressure

The correct holding pressure depends on gate geometry, wall thickness, mold temperature, material grade, screw size, and machine pressure display. The following ranges are starting values for common injection molding materials. They assume the controller is displaying melt pressure in the screw or cavity. If the machine displays hydraulic pressure, the set values will be different. Always confirm the pressure scale used by the molding machine before comparing settings.

MaterialTypical melt holding pressure range (MPa)Typical holding time per mm wallMain risk if pressure is too lowMain risk if pressure is too high
PP25–55 MPa0.3–0.5 s/mmSink marks, low part weight, dimensional driftFlash, warpage, ejection stress
ABS30–70 MPa0.3–0.6 s/mmSink marks, dull surface, unstable dimensionsOverpack near gate, warpage, difficult ejection
PC60–100 MPa0.4–0.8 s/mmVoids, poor surface quality, dimensional variationResidual stress, stress cracking, ejection marks
POM50–90 MPa0.3–0.5 s/mmSink marks, shrinkage, voids in thick sectionsFlash, warpage, gate-area stress
PA6650–90 MPa0.3–0.6 s/mmSink, shrinkage, poor dimensional stabilityFlash, warp, overpacking in thin sections

Use these only as a first trial. The final setting must be validated against actual shot weight, dimensional readings, surface quality, and cycle stability on the production mold.

How to Set Holding Pressure: Step-by-Step Process Guide

Holding pressure should never be copied from another mold. The sequence below is the practical process used during mold validation and troubleshooting: start with a stable fill, find the gate seal point, adjust pressure in small steps, and confirm with part weight.

1. Verify the switchover position first

Before adjusting holding pressure, make sure the cavity is filled in a controlled way. Run short shots to identify the switchover position where the part is nearly complete but not overfilled. If the switchover happens too late, the screw packs the part during the fill stage, and holding pressure starts with an already overpacked cavity. If switchover happens too early, the holding stage is forced to do filling work, which creates unstable pressure and weight variation. A small cushion should remain in front of the screw during holding.

2. Run a gate seal test

Set an initial holding pressure and a short holding time. Run enough cycles to stabilize melt temperature, then measure the average shot weight as you increase holding time in 1-second steps. When the average part weight stops increasing, the gate has sealed. Add 0.5–1.0 seconds of holding time as a production safety margin.

  • Measure 5–10 shots for each holding time condition and use the average weight.
  • Increase holding time one second at a time, not by large jumps.
  • Stop when the weight increase between two steps is close to zero or less than the scale repeatability.
  • Record the gate seal time for future process reference.

Gate seal time is specific to the gate size, wall thickness, melt temperature, and mold temperature. Two different molds running the same material can have completely different holding time requirements.

3. Adjust pressure and inspect defects

Start with the relevant range from the table. If the part has sink marks, raise holding pressure in steps of 5–10 MPa and recheck shot weight. If flash appears, check clamp force, venting, and mold fit before simply lowering the pressure. After every pressure change, run enough cycles for the process to stabilize. Do not judge a change after only one or two shots.

Use strong, angled light to check sink marks on surfaces. Measure critical dimensions only after the part has reached a stable temperature. A part measured immediately after ejection can give a misleading dimension or flatness reading.

4. Confirm with part weight and cavity balance

Part weight is one of the most reliable indicators of holding pressure. If the shot weight shifts after a pressure setting is changed, packing has changed. Define a practical shot weight tolerance for the production run, not just a single nominal value.

In multi-cavity molds, measure each cavity separately if possible. If one cavity sinks and another flashes under the same pressure, the problem is often gate balance or feed system design. A single machine pressure value cannot fix uneven cavities.

One Holding Pressure Setting Is Usually Not Enough

Injection molding holding pressure works against a gate that changes resistance as the polymer cools. A constant pressure may be acceptable for a simple part, but many production parts benefit from a two-stage pressure profile.

A typical profile uses a higher packing pressure for the first short phase, while the gate is still fully open, to pack out the surface and tight dimensions. The second phase uses a lower holding pressure to maintain material contact without overpacking the gate area. Some thin-wall or long-flow parts need a more gradual three-stage profile to balance pressure delivery.

The purpose is not to make the process complex. It is to match pressure to the changing behavior of the melt in the mold.

Common Holding Pressure Mistakes and How to Detect Them

  • Using holding pressure to fix short shots. Check shot size, switchover position, and cushion first.
  • Copying settings from an existing mold. Gate design, wall thickness, and cavity layout change the required holding pressure completely.
  • Setting holding time too short. Symptom: lot-to-lot weight variation, sink marks under the gate, and dimension drift.
  • Setting holding time too long. Cycle time increases, but part weight no longer changes. The additional time is wasted.
  • Ignoring an unstable cushion. If cushion size moves between cycles, holding pressure cannot be delivered consistently. Check the non-return valve and barrel temperature profile.
  • Raising pressure without checking tool condition. Flash and ejection marks may reappear after the mold has worn, even if pressure has not changed.

What Buyers and Engineers Should Ask About Holding Pressure

When evaluating a mold supplier or production factory, holding pressure is not a secret parameter. It can be documented in mold trial reports and process sheets. A mature manufacturing process should show pressure values, holding time, shot weight data, and validation results together.

For a sourcing project, ask practical questions before accepting a process card:

  • What holding pressure profile is used for this tool, and why was that profile selected?
  • Was gate seal time measured, or was holding time copied from a similar part?
  • What is the part weight tolerance, and how is shot weight monitored during production?
  • How does the mold behave at the upper pressure limit in terms of flash, ejection, and clamp tonnage?
  • At what conditioning time after ejection were the dimensional measurements taken?

These details are more useful than a holding pressure value in a quotation. They show whether the supplier understands the process or simply filled in a number on a checklist.

Get the switchover right. Set a starting pressure. Find the gate seal time. Adjust in small steps. Confirm with part weight and dimension. Once those controls are in place, holding pressure stops being a guess and becomes a repeatable part of the production process.